The 3D filament Kimya ASA-S belongs to the styrenic polymer family. Acrylonitrile styrene acrylate (ASA) is an opaque thermoplastic terpolymer. ASA offers properties close to ABS but is suitable for long-term external use. Its resistance to climatic conditions provides it with durability over time. ASA is notably used in the automotive industry.
- High weather resistance
- High UV resistance
- Complies with the RoHS and REACH standards
Technical Information
FILAMENT PROPERTIES
PROPERTIES | TEST METHODS | VALUES |
---|---|---|
Diameter | INS-6712 | 1.75 ± 0.1 mm |
Density | ISO 1183-1 | 1.056 g/cm3 |
Moisture rate | INS-6711 | < 1 % |
Melt flow index (MFI) | ISO 1133-1 (@220°C 10 kg) | 4 - 10 g/10min |
Glass transition temperature (Tg) | ISO 11357-1 DSC (10°C/min - 20-300°C) | 108 °C |
PRINT PARAMETERS AND SPECIMENS DIMENSIONS
PRINTING DIRECTION | XY |
---|---|
Printing Speed | 20-60 mm/s |
Infill | 100% - rectilinear |
Infill Angle | 45°/-45° |
Nozzle Temperature | 240-260°C |
Bed T° | 90-100°C |
PRINTED SPECIMENS PROPERTIES
PROPERTIES | TEST METHODS | VALUES | |
---|---|---|---|
MECHANICAL PROPERTIES | |||
Tensile modulus | ISO 527-2/5A/50 | 1,685 MPa | |
Tensile Strength | ISO 527-2/5A/50 | 38 MPa | |
Tensile strain at strength | ISO 527-2/5A/50 | 2 % | |
Tensile Stress at Break | ISO 527-2/5A/50 | 34.6 MPa | |
Tensile strain at break | ISO 527-2/5A/50 | 4 % | |
Flexural modulus | ISO 178 | 1,662 MPa | |
Flexural strength* | ISO 178 | <5 % | |
Flexural stress at conventional deflection (3,5% strain)* | ISO 178 | 57.3 MPa | |
Charpy impact resistance | ISO 179-1/1eA | 13 kJ/m² | |
Shore Hardness | ISO 868 | 74D |
Note 1 *According to ISO 178, end of the test at 5% deformation even if there is no specimen break.
Note 2 The data should be considered as indicative values - Properties can be influenced by production conditions.
Print Setting
- Print speed: 20-60 mm/s
- Extrusion temperature: 240-260°C
- Platform temperature: 90-100°C
Miscellaneous
Highlight 2 | Abrasion And Uv Resistance |
Spool Material | PC |
Steaming Temperature | 80°C |